ASTM B709

This specification covers iron-nickel-chromiummolybdenum alloy (UNS N08028)* plate, sheet, and strip in the solution-annealed condition. This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility of the user of this standard to become familiar with all hazards including those identified in the appropriate Material Safety Data Sheet for this product/material as provided by the manufacturer, to establish appropriate safety and health practices, and determine the applicability of regulatory limitations prior to use.

Chemical Properties

Ni Fe Cr Mo C, max Si, max Mn, max P, max S, max Cu
29.5-32.5 remainderA 26.0-28.0 3.0-4.0 0.030 1.00 2.50 0.030 0.030 0.6-1.4
Note A: Determined arithmetically by difference

Mechanical Properties

Form Tensile Strength, min,
ksi (MPa)
Yield Strength (0.2 % offset), min,
ksi (MPa)
Elongation in 2 in. or 50 mm, or 4D, min,
%
Rockwell Hardness (or equivalent)A
Sheet 73 (500) 31 (214) 40 70–90 HRB
Strip 73 (500) 31 (214) 40 70–90 HRB
Plate 73 (500) 31 (214) 40 70–90 HRB
Note A: Hardness values are shown for information only and shall not constitute a basis for acceptance or rejection as long as the other mechanical properties are met.