ASTM A193 Grade B8LN Class 1D is a standard material specification for nitrogen enhanced corrosion resistant 304LN stainless steel fasteners, for use in high tensile, high temperature and special purpose applications such as pressure piping & pressure vessels bolting. Grade B8LN Class 1D is a carbide solution treated 304LN stainless steel having a minimum tensile requirement of 75 ksi, yield 30 ksi and maximum hardness limit of 223 HBW or 96 HRB. ASTM A193 specification covers requirements for chemical composition, mechanical properties, hardness, heat-treatment and recommended nuts-washers for Grade B8LN Class 1D Fasteners.
Element | Austenitic Stainless Steel |
---|---|
AISI 304LN / UNS S30453 | |
CompositionA, % | |
Carbon | 0.03 max |
Manganese | 2.00 |
Phosphorus | 0.045 max |
Sulfur | 0.030 max |
Silicon | 1.00 max |
Chromium | 18.00 - 20.00 |
Nickel | 8.00 - 11.00 |
Nitrogen | 0.10 - 0.16 |
A; The intentional addition of Bi, Se, Te, and Pb is not permitted.
Tensile Class | Diameter, Inch | Tensile Strength, min, ksi |
Yield Strength, min, 0.2% offset, ksi |
Elongation in 4D, min, % |
Reduction of Area, min, % |
Hardness, maxA |
|
---|---|---|---|---|---|---|---|
Class 1D | All Sizes | 75 | 30 | 30 | 50 | 223 HBW or 96 HRB |
Heat Treatment: Carbide Solution Treated
A: For sizes 3⁄4 in. in diameter and smaller, a maximum hardness of 241 HBW (100 HRB) is permitted.